MA601 | Heat Resistance Alloys
Ni-23Cr-14Fe-1.35Al (mass%)
Nickel chrome alloy featuring outstanding aspects both in corrosion resistance and heat resistance
Main Features
MA601 is resistant to high temperature oxidizing atmosphere up to 1205°C, and has excellent carburizing resistance. The oxidation resistance is mainly achieved by chrome, and the relatively high aluminum content of this alloy further improves the oxidation resistance.Mainly used for heating furnace, heat treatment furnace, thermocouple protective tube, glow plug, gasoline engine thermal reactor, petrochemical industry heater, etc.
Weldability/Workability
Molding process and welding can be easily performed.Use INCO-WELD A, INCONEL WELDING ELECTRODE182 for arc welding. Use INCONEL FILER METAL 82, INCONEL FILER METAL 601 for TIG.
INCONEL, INCO-WELD are registered trademarks of Special Materials Corporation.
Available Product Forms
Various shapes, such as flat-rolled plates, forgings, welding wire, wire, welded pipes and tubes, seamless pipes and tubes can be manufactured.
Specifications
Information on specifications to which MA601 alloy can be ordered.
ASTM UNS N06601
| Plates |
Bars, Wires |
Pipes and Tubes |
| B168 |
B166 |
B163 |
| |
B564 |
B167 |
ASME UNS N06601
| Plates |
Bars, Wires |
Pipes and Tubes |
| SB168 |
SB-166 |
SB-163 |
| |
|
SB-167 |
Code Case 1500
JIS NCF601
| Plates |
Bars, Forgings |
| G4902 |
G4901 |
AMS UNS N06601
| Plates |
Bars, Forgings |
| 5870 |
5715 |
Mechanical Properties
Room temperature tensilty
| Shape |
Tensile strength/ N/mm2 |
Yield strength (0.2%expansion) N/mm2 |
Elongation % |
Hardness(HB) |
| Bar |
700 |
305 |
45 |
160∼179 |
| Plate |
700 |
305 |
42 |
HRB 81∼92 |
High temperature tensilty
| Temperature°C |
Tensile strength, N/mm2 |
Yield strength (0.2%expansion) N/mm2 |
Elongation % |
| 538 |
590 |
160 |
50 |
| 649 |
510 |
175 |
47 |
| 760 |
290 |
190 |
78 |
| 871 |
150 |
130 |
91 |
| 982 |
90 |
70 |
100 |
Creep rupture
| Temperature°C |
1000hrs strength N/mm2 |
10,000hrs strength N/mm2 |
| 649 |
193.2 |
137.3 |
| 760 |
62.8 |
34.3 |
| 871 |
29.4 |
17.7 |
| 982 |
14.7 |
7.8 |